搅拌站混凝土及原材料检验规程目录混凝土检验规程................................................................................01.混凝土拌合物性能试验方法..............................................02.立方体抗压强度试验..........................................................13.混凝土抗渗试验..................................................................34.混凝土含气量测定实验......................................................55.混凝土抗冻融实验..............................................................76.混凝土凝结时间测定实验..................................................7水泥检验规程..................................................................................121.取样....................................................................................122.标准稠度用水量的测定(用不变水量法)....................123.凝结时间的测定(人工测定)........................................134.安定性................................................................................145.水泥胶砂强度....................................................................156.水泥胶砂流动度................................................................18外加剂检验规程..............................................................................201.取样....................................................................................202.外加剂性能测定:............................................................203.外加剂匀质性....................................................................25粉煤灰检验规程..............................................................................341.取样....................................................................................342.烧失量测定方法................................................................343.含水率测定方法................................................................354.细度测定方法....................................................................355.需水量比测定方法............................................................36粒化高炉矿渣粉检验规程..............................................................381.取样....................................................................................382.矿粉的技术指标................................................................383.比表面积的测定(勃氏法)............................................384.矿粉活性指数的测定........................................................415.矿渣粉的流动度比试验....................................................42砂检验规程.......................................................................................431.取样....................................................................................432.筛分析试验........................................................................433.含泥量试验(标准法)....................................................454.泥块含量试验....................................................................465.含水率试验........................................................................47石检验规程.......................................................................................491.取样....................................................................................492.颗粒级配试验....................................................................493.含泥量试验........................................................................504.泥块含量试验....................................................................515.针片状颗粒含量试验........................................................526.含水率试验........................................................................537.石子压碎指标值的测定....................................................54混凝土检验规程1.混凝土拌合物性能试验方法1.1拌合物取样及试样制备混凝土拌合物试验用料应根据不同要求,从同一盘搅拌或同一车运送的混凝土中取出,或在试验室用机械或人工单独拌制,取样量应多于试验所需的1.5倍,且不应少于20升。1.2稠度试验(坍落度法)1.2.1准备工作:湿润铁盘、铁锨、小铲、捣棒、坍落度筒并把筒放在不吸水的水平钢板上,使坍落度筒在试验过程中保持位置固定。1.2.2试验步骤:(1)将混凝土拌合物用小铲分三层均匀地装入筒中,使捣实后每层高度为筒高的1/3左右,每层用捣棒捣25次,插捣时沿坍落度筒壁按螺旋方向由外向中心进行。各次插捣应在截面上均匀分布,插捣底层时,捣棒应贯穿整个深度,插捣第二层和第三层时,捣棒应插透本层至下一层的表面。顶层插捣完后,用抹刀刮去多余的混凝土,并抹平;(2)除去筒边底板上的混凝土后,垂直平稳地提起坍落度筒,坍落度筒的提高过程应在5~10s内完成,从开始装料到提高坍落度筒的整个过程应不间断地进行,并在150s之内完成;(3)提起坍落度筒后,用混凝土尺台测量坍落后试体最高点,直接读出该拌合物的坍落度值,数值以毫米为单位,精确至5mm。1.2.3评定:(1)坍落度筒提起后,如果混凝土发生崩坍或一边剪坏现象,需重新取样后另行测定,如第二次试验仍出现上述现象,则表示该混凝土和易性不好,应予记录备查;(2)观察坍落度后的混凝土试体粘聚性及保水性,粘聚性的检查方法是用捣棒在已坍落的混凝土锥体侧面轻轻敲打,此时,如果锥体逐渐下沉,表示粘聚性较好,如果锥体倒坍,则表示粘聚性不好;(3)当坍落度筒提起后,如果有较多的稀浆从底部析出,锥体部分的混凝土也因失浆而集料外露,则表明此混凝土拌合物的保水性能不好。2.立方体抗压强度试验2.1试块留置:对相同原材料、相同混凝土配合比、相同混凝土等级、相同混凝土生产工艺的混凝土每100m3取样不得少于一组。如连续浇筑1000m3以上,则每200m3取样不得少于一组。应在浇筑地点当车卸料量的1/4~3/4处随机取样制作。2.2试块的制作:2.2.1混凝土拌合物应分两层装入试模,每层的装料厚度大致相等。插捣时按螺旋方向从边缘向中心均匀进行,插捣底层时,捣棒应达到试模底面,插捣上层时,捣棒应穿入下层深度为20~30mm,插捣时捣棒要保持垂直,不得倾斜。同时还要用抹刀沿试模内壁插入数次。每回插捣次数不少于12次。插捣完后,刮去多余的混凝土,并抹平;2.2.2试块成型后应覆盖表面以防止水份蒸发,静置条件为20±5℃,时间为一昼夜至二昼夜。2.2.3用震动台成型时,应将混凝土拌合物一次装入试模,装料时应用抹刀沿试模内壁插捣并使混凝土拌合物高出试模上口。振动时应防止试模在震动台上自由跳动。震动应持续到混凝土表面出浆为止,刮除多余的混凝土,待混凝土邻近初凝时用抹刀抹平。2.3试块的养护:拆模后的试件应及时编号,在温度为20±2℃,相对湿度为95%的标准养护室进行标准养护,试件之间应彼此间隔10-20mm,同时应保证试件表面保持潮湿且不被水直接冲淋。2.4立方体抗压强度试验步骤:2.4.1试压时先将试块表面擦干并测量尺寸,当一组对边实际边长未超过标准值的1%时,该边长取标准值,而试块受压面积则取测量后的实际面积;2.4.2检查试块外观,选择比较平整且垂直的非浇筑面进行试验;2.4.3根据混凝土强度等级,确定压力机度盘(有效值20%~80%)及加荷速度:混凝土强度等级加荷速度每秒<C300.3~0.5N/mm2≥C30且<C600.5~0.8N/mm2≥C600.8~1.0N/mm22.4.4将试块放在压力机的下压板上,试块的受压面应与试块成型时的顶面垂直,试块的中心应与试验机下压板中心对准,开动压力机,当上压板与试块接近时,调整球座,使其接触均衡,混凝土试块压力试验应连续而均匀地加荷,当试块接近破坏而开始